TDS comparison
| Property | 50100 GS Caltex | BU7100 Lotte Chemical | HD12500 SIBUR | B4660 SABIC |
|---|---|---|---|---|
| Melt flow (190 °C/21.6 kg) | 9.75 g/10 min | 10 g/10 min | 12 g/10 min | 46 g/10 min |
| Density | 0.948 g/cm³ | 0.948 g/cm³ | 0.951 g/cm³ | 0.961 g/cm³ |
| Tensile strength at yield | 25 MPa | 260 kg/cm² (≈25.5 MPa) | 23 MPa | 30 MPa |
| Flexural modulus | 1200 MPa | 11200 kg/cm² (≈1,099 MPa) | — | 1100 MPa |
| ESCR | 1000 h | > 1000 h | — | — |
| Vicat softening point | 126 °C | — | — | 127 °C |
| Elongation at break | — | — | 700 % | — |
| Notched Charpy impact (23 °C) | — | — | 14 kJ/m² | — |
| Melt flow (190 °C/2.16 kg) | — | — | — | 0.7 g/10 min |
Typical values from each producer's TDS, for reference only, not guaranteed specifications. "—" means not stated on the TDS. Values marked "≈" are unit conversions by Thien An for easier comparison.
Key differences
- 50100 (GS Caltex) and BU7100 (Lotte) are almost equivalent: HLMI 9.75 and 10, density 0.948, ESCR from 1,000 h, tensile 25 and ≈25.5 MPa.
- HD12500 (SIBUR) has HLMI 12, for extrusion and blow molding, with 14 kJ/m² Charpy and 700 % elongation.
- B4660 (SABIC) is a high-density homopolymer (0.961), stiffer (30 MPa tensile) and much faster flowing (HLMI 46) – for stiff bottles and small cans rather than large parts.
- Large parts need low melt flow.
Which grade to choose?
- Large cans, drums: 50100 or BU7100 – interchangeable.
- Extrusion plus blow molding needing toughness: HD12500.
- Stiff bottles and small cans: B4660.
Tips when switching grades
- Compare like with like: same test method and units (ISO/ASTM; MPa or kg/cm²; Izod or Charpy). Values from different methods are not directly comparable.
- Melt flow has a lot-to-lot tolerance – check the COA of the actual lot, not just the TDS.
- Different additives (nucleating, antistatic, antioxidant, slip) can change the part even when key values match.
- Always trial on your own machine and mold: check temperature, pressure, shrinkage, colour and appearance before switching volume.
FAQ
What is HLMI and how does it differ from MI?
HLMI is melt flow at 21.6 kg load, MI at 2.16 kg. Large blow-molding grades flow very slowly, so producers usually report HLMI.
Can 50100 and BU7100 replace each other?
Per TDS their HLMI, density and ESCR are almost identical, so usually yes; trial to adjust temperature and blow time.
Can B4660 make large cans?
B4660 flows much faster (HLMI 46), so the parison sags more for large parts. It suits stiffer bottles and small cans.
Grade pages with TDS downloads: 50100 · BU7100 · HD12500 · B4660
Other comparisons: LDPE film grades · LLDPE film grades · HDPE film grades · HDPE injection grades by melt flow · HDPE pipe grades · HDPE for monofilament, nets and tape