LDPE film grades: FD0270 vs FD0274 vs FD0474 vs 4025AS
Four LDPE grades with density 0.923–0.925 g/cm³, all for blown film. They differ mainly in melt flow (2.4 or 4) and in whether they contain slip and antiblock additives.
Updated: 17 Nov 2026 · Thien An Plastics
TDS comparison
| Property | FD0270 Qatar Petrochemical (QAPCO) | FD0274 Lotrène (Qatar) | FD0474 Lotrène (Qatar) | 4025AS Tasnee |
|---|---|---|---|---|
| Melt flow (190 °C/2.16 kg) | 2.4 g/10 min | 2.4 g/10 min | 4 g/10 min | 4 g/10 min |
| Density | 0.923 g/cm³ | 0.923 g/cm³ | 0.923 g/cm³ | 0.925 g/cm³ |
| Melting point | 112 °C | 108 °C | 108 °C | 111 °C |
| Vicat softening point | 96 °C | 89 °C | 87 °C | 92 °C |
| Haze | 5.5 % | 8 % | 7 % | < 9 % |
| Dart impact | — | 110 g | 90 g | 100 g |
Typical values from each producer's TDS, for reference only, not guaranteed specifications. "—" means not stated on the TDS. Values marked "≈" are unit conversions by Thien An for easier comparison.
Key differences
- The MFR 2.4 pair (FD0270, FD0274) gives tougher film: FD0274 dart is 110 g versus 90 g for FD0474 (MFR 4) from the same brand.
- The MFR 4 pair (FD0474, 4025AS) flows more easily – better for thin film and high output.
- 4025AS already contains slip and antiblock – film opens easily; FD0270 is additive-free – suited to printing, lamination or your own masterbatch.
- Haze ranges from 5.5 % (FD0270) to below 9 % (4025AS) per TDS; compare only at the same film thickness and method.
Which grade to choose?
- Bags and film needing toughness: FD0274 or FD0270.
- Thin film at high output: FD0474.
- Automatic packaging needing non-blocking film: 4025AS.
- Film for printing, lamination or own additives: FD0270.
Tips when switching grades
- Compare like with like: same test method and units (ISO/ASTM; MPa or kg/cm²; Izod or Charpy). Values from different methods are not directly comparable.
- Melt flow has a lot-to-lot tolerance – check the COA of the actual lot, not just the TDS.
- Different additives (nucleating, antistatic, antioxidant, slip) can change the part even when key values match.
- Always trial on your own machine and mold: check temperature, pressure, shrinkage, colour and appearance before switching volume.
FAQ
How do LDPE MFR 2 and MFR 4 differ?
Lower MFR (about 2) gives tougher film; higher MFR (about 4) flows better, suits thin film and faster output but the film is less tough.
Do I need LDPE with slip and antiblock?
Yes if film layers stick together or run on automatic packaging lines. For printed or laminated film, use an additive-free grade so ink and adhesive bond well.
Can FD0274 and FD0270 replace each other?
Both are MFR 2.4 with density 0.923, so usually yes; run a film trial to check clarity and toughness.
Grade pages with TDS downloads: FD0270 · FD0274 · FD0474 · 4025AS
Other comparisons: LLDPE film grades · HDPE film grades · HDPE injection grades by melt flow · HDPE pipe grades · HDPE for large blow-molded parts · HDPE for monofilament, nets and tape
Based on producers' public TDS, for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).