Properties from the TDS
| Property | UI2420 SCG Chemicals (Thailand) | UI2650 SCG Chemicals (Thailand) | UL814 Lotte Chemical | DNDA-8320 Luban (OQ, Oman) | LL 6100 ExxonMobil | LL 6201.19 ExxonMobil | M200024 SABIC | HM2420 Sasol |
|---|---|---|---|---|---|---|---|---|
| Melt index (190 °C/2.16 kg) | 20 g/10 min | 50 g/10 min | 20 g/10 min | 20 g/10 min | 20 g/10 min | 50 g/10 min | 20 g/10 min | 20 g/10 min |
| Density | 0.924 g/cm³ | 0.927 g/cm³ | 0.924 g/cm³ | 0.924 g/cm³ | 0.925 g/cm³ | 0.926 g/cm³ | 0.924 g/cm³ | 0.924 g/cm³ |
| Comonomer | — | — | Butene | Butene | Butene | Butene | — | Hexene |
| Vicat softening point | 90 °C | 90 °C | — | — | 87 °C | — | — | — |
| Tensile strength at yield | — | — | 10.3 MPa | — | 13 MPa | — | — | 15 MPa |
| Flexural modulus | — | — | — | — | 480 MPa (1% secant) | — | — | 440 MPa |
| ESCR (conditions per TDS) | 24 h | 30 h | — | — | 110 h (F50, 10% Igepal) | — | — | — |
Typical values from each producer's TDS, for reference only and not specifications. "—" means not published in the TDS. Values marked "≈" were converted by Thien An for easier comparison.
Key differences
- Two melt-flow groups: MI 20 (UI2420, UL814, DNDA-8320, LL 6100, M200024, HM2420) and MI 50 (UI2650, LL 6201.19). MI 50 flows very easily for thin-wall parts and long flow paths; MI 20 gives tougher, more crack-resistant parts.
- Almost identical density (0.924–0.927 g/cm³), so stiffness is similar across all eight.
- HM2420 is a hexene LLDPE; UL814, DNDA-8320, LL 6100 and LL 6201.19 are butene LLDPE. Sasol positions HM2420 for high gloss and good low-temperature impact.
- ESCR is not directly comparable: LL 6100 lists 110 h (F50, 10% Igepal), while UI2420/UI2650 list 24 h and 30 h under different test conditions.
- ExxonMobil has renamed LL 6100 as C4LL 20025.17; the old name is still widely used.
Which grade to choose?
- Caps, lids, general flexible housewares: the MI 20 group – UI2420, UL814, DNDA-8320, LL 6100 and M200024 are usually interchangeable after a trial run.
- High gloss and good cold impact: HM2420 (hexene).
- Very thin parts, multi-cavity moulds, masterbatch carriers: the MI 50 group – UI2650, LL 6201.19.
- Outdoor parts: the UI2420/UI2650 TDS states no UV stabiliser – add a UV additive.
Notes when switching grades
- Do not swap between MI 20 and MI 50 without re-adjusting temperature, pressure and hold time.
- Compare like-for-like test methods (ASTM/ISO) and ESCR conditions.
- Check the COA of the actual lot and run a trial on your own mould before switching volume.
FAQ
Are UI2420, UL814 and M200024 interchangeable?
Usually yes for general injection parts, as all are MI 20 with density 0.924 g/cm³. Run a trial, since additives and molecular distribution differ by producer.
How does injection LLDPE differ from injection HDPE?
LLDPE is more flexible, tougher and more crack-resistant; HDPE is stiffer. Caps opened many times and flexible parts usually use LLDPE.
When should I use MI 50 LLDPE?
For very thin parts, long flow paths or masterbatch carriers – e.g. UI2650 or LL 6201.19.
Is the TDS available?
Yes. Each grade page on thienanplastics.com has the TDS for download.
Grade pages (TDS download): UI2420 · UI2650 · UL814 · DNDA-8320 · LL 6100 · LL 6201.19 · M200024 · HM2420
More articles: HDPE injection grades by melt flow · LLDPE film grades: FS253S, HB18N, HP1018BN, LLD7050 · PP homopolymer injection grades, MFR 12
Based on producers' public TDS; for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).