High-flow PP for thin-wall injection: J1105T vs J1102T vs BX3900 vs AX161 vs PPH-G75T
Thin-wall food containers, cups and lids need very high-flow PP for fast filling and short cycles. The key choice is homopolymer (stiffer, clearer) or impact copolymer (tougher, better in the cold).
Updated: 17 Nov 2026 · Thien An Plastics
TDS comparison
| Property | J1105T Hyosung (Topilene) | J1102T Hyosung | BX3900 SK Geo Centric | AX161 TPC (Singapore) | PPH-G75T Dongguan Grand Resource |
|---|---|---|---|---|---|
| Melt flow (230 °C/2.16 kg) | 60 g/10 min | 60 g/10 min | 61 g/10 min | 65 g/10 min | 75 g/10 min |
| Density | 0.9 g/cm³ | 0.9 g/cm³ | — | 0.9 g/cm³ | — |
| Tensile strength at yield | 350 kg/cm² (≈34.3 MPa) | — | — | 30 MPa | — |
| Flexural modulus | 18000 kg/cm² (≈1,766 MPa) | — | — | 1415 MPa | — |
| Notched Izod impact (23 °C) | 4 kg·cm/cm (≈39.2 J/m) | — | — | 59 J/m | — |
| Rockwell hardness (R) | — | — | — | 97 | — |
| HDT (0.45 MPa) | — | — | — | 129 °C | — |
Typical values from each producer's TDS, for reference only, not guaranteed specifications. "—" means not stated on the TDS. Values marked "≈" are unit conversions by Thien An for easier comparison.
Key differences
- Homopolymers: J1105T, J1102T (Hyosung, MFR 60) and PPH-G75T (Dongguan, MFR 75). J1105T reports flexural modulus 18,000 kg/cm² (≈1,770 MPa) – very stiff – but Izod only ≈39 J/m.
- Impact copolymers: AX161 (TPC, MFR 65) with 59 J/m Izod, HDT 129 °C and 1,415 MPa modulus; BX3900 (SK, MFR 61) is classified as a high-crystallinity copolymer.
- Some TDS (J1102T, PPH-G75T, BX3900) give few properties – trial to compare stiffness and warpage.
Which grade to choose?
- Containers and cups needing stiffness with little impact: J1105T, J1102T, PPH-G75T.
- Freezer containers and parts that may be dropped: AX161 or BX3900 (copolymers are tougher in the cold).
- Food-contact parts: request food-contact certificates per grade and lot.
Tips when switching grades
- Compare like with like: same test method and units (ISO/ASTM; MPa or kg/cm²; Izod or Charpy). Values from different methods are not directly comparable.
- Melt flow has a lot-to-lot tolerance – check the COA of the actual lot, not just the TDS.
- Different additives (nucleating, antistatic, antioxidant, slip) can change the part even when key values match.
- Always trial on your own machine and mold: check temperature, pressure, shrinkage, colour and appearance before switching volume.
FAQ
Homopolymer or copolymer for thin-wall molding?
Homopolymer is stiffer, clearer and usually cheaper; copolymer is tougher and better for cold and drops. Use copolymer for freezer containers.
How do MFR 60 and 75 differ?
MFR 75 flows faster, suiting very thin walls or many cavities, but toughness is usually lower – trial first.
How do J1105T and J1102T differ?
Same producer, same MFR 60. The J1105T TDS gives stiffness and impact, the J1102T TDS gives few properties – ask the producer or trial to compare.
Grade pages with TDS downloads: J1105T · J1102T · BX3900 · AX161 · PPH-G75T
Other comparisons: LDPE film grades · LLDPE film grades · HDPE film grades · HDPE injection grades by melt flow · HDPE pipe grades · HDPE for large blow-molded parts
Based on producers' public TDS, for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).