PP impact copolymer for injection, MFR 9: B350F vs AW161 vs C080MA vs UE400M vs J646H
Five grades with the same melt flow of 9 g/10 min, all for impact-resistant injection parts. The difference lies in the balance between stiffness and impact toughness – which decides whether a part feels rigid or survives drops.
Updated: 17 Nov 2026 · Thien An Plastics
TDS comparison
| Property | B350F SK Geo Centric (Korea) | AW161 TPC (Singapore) | C080MA Reliance (India) | UE400M DaelimPoly (Korea) | J646H Hyosung (Korea) |
|---|---|---|---|---|---|
| Melt flow rate (230 °C/2.16 kg) | 9 g/10 min | 9 g/10 min | 9 g/10 min | 9 g/10 min | 9 g/10 min |
| Tensile strength at yield | 270 kg/cm² (≈26 MPa) | 28.5 MPa | 23 MPa | 270 kg/cm² (≈26 MPa) | 270 kg/cm² (≈26 MPa) |
| Flexural modulus | 12,000 kg/cm² (≈1,180 MPa) | 1,170 MPa | 1,000 MPa | 11,000 kg/cm² (≈1,080 MPa) | 13,500 kg/cm² (≈1,320 MPa) |
| Notched Izod impact (23 °C) | 12 kg·cm/cm (≈118 J/m) | 75 J/m | 150 J/m | 15 kg·cm/cm (≈147 J/m) | — |
| HDT (0.45 MPa) | — | 117 °C | — | — | 115 °C |
| Vicat softening point | 150 °C | — | — | — | — |
| Rockwell hardness (R) | 90 | 90 | — | — | — |
| Shore D hardness | — | — | 68 | — | — |
Typical values from each producer's TDS, for reference only, not guaranteed specifications. "—" means not stated on the TDS. Values marked "≈" are unit conversions by Thien An for easier comparison.
Key differences
- Same MFR 9, but flexural modulus ranges from ≈1,000 MPa (C080MA) to ≈1,320 MPa (J646H), and Izod impact from 75 J/m (AW161) to 150 J/m (C080MA).
- General rule: stiffer grades tend to be less impact-tough, and vice versa. C080MA is the toughest but softest; J646H and AW161 are stiffer and more heat resistant (HDT 115–117 °C).
- B350F and UE400M are balanced: impact ≈118–147 J/m, modulus ≈1,080–1,180 MPa.
- C080MA is classified by its producer as antistatic – keep this in mind when replacing it in parts that must resist dust.
Which grade to choose?
- Parts that must survive drops and heavy impact (crates, boxes, housewares): prefer C080MA, UE400M, B350F.
- Parts needing stiffness and low deformation when warm: prefer J646H, AW161.
- When substituting, match both modulus and impact (e.g. B350F ↔ UE400M), not just MFR.
Tips when switching grades
- Compare like with like: same test method and units (ISO/ASTM; MPa or kg/cm²; Izod or Charpy). Values from different methods are not directly comparable.
- Melt flow has a lot-to-lot tolerance – check the COA of the actual lot, not just the TDS.
- Different additives (nucleating, antistatic, antioxidant, slip) can change the part even when key values match.
- Always trial on your own machine and mold: check temperature, pressure, shrinkage, colour and appearance before switching volume.
FAQ
Are PP impact copolymers with the same MFR 9 the same?
Not really. MFR only describes flow. Per their TDS, stiffness and impact differ significantly among these five, so choose by part requirements and run a trial.
Which grade is toughest?
Per TDS, C080MA (150 J/m) and UE400M (≈147 J/m) have the highest Izod impact in this group.
Which grade is stiffest?
J646H has the highest flexural modulus (≈1,320 MPa), followed by B350F and AW161.
Grade pages with TDS downloads: B350F · AW161 · C080MA · UE400M · J646H
Other comparisons: PP homopolymer for injection, MFR 12 · Are "5502" HDPE blow-molding grades from different producers the same? 5502 vs 5502BN vs Q5502BN vs HY55430 · Clear random PP for injection · General-purpose injection ABS
Based on producers' public TDS, for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).