Clear random PP for injection: R380Y vs R801N vs RJ870Z
Random PP copolymer is used for clear injection parts: containers, cups, clear housewares. The three Korean grades below have melt flow of 29–40.
Updated: 17 Nov 2026 · Thien An Plastics
TDS comparison
| Property | R380Y SK Geo Centric | R801N Hyosung (Topilene) | RJ870Z Hanwha TotalEnergies |
|---|---|---|---|
| Melt flow rate (230 °C/2.16 kg) | 29 g/10 min | 30 g/10 min | 40 g/10 min |
| Density | — | — | 0.90 g/cm³ |
| Tensile strength at yield | 300 kg/cm² (≈29 MPa) | 290 kg/cm² (≈28 MPa) | — |
| Flexural modulus | 12,000 kg/cm² (≈1,180 MPa) | 11,000 kg/cm² (≈1,080 MPa) | — |
| Notched Izod impact (23 °C) | 4 kg·cm/cm (≈39 J/m) | 7 kg·cm/cm (≈69 J/m) | — |
| HDT (0.45 MPa) | — | 90 °C | 95 °C |
| Vicat softening point | 135 °C | — | — |
| Rockwell hardness (R) | — | — | 85 |
| Haze | 10 % | — | 18 % |
Typical values from each producer's TDS, for reference only, not guaranteed specifications. "—" means not stated on the TDS. Values marked "≈" are unit conversions by Thien An for easier comparison.
Key differences
- R380Y and R801N are close in MFR (29–30) and tensile strength; R801N is tougher (≈69 vs ≈39 J/m), R380Y slightly stiffer.
- RJ870Z flows more (MFR 40) – better for thin walls and faster cycles.
- Haze of 10 % (R380Y) and 18 % (RJ870Z) can only be compared at the same specimen thickness and method; producers often test different specimens.
- Hyosung lists R801N for injection stretch blow molding (ISBM) as well – useful if the plant also makes clear bottles.
Which grade to choose?
- Boxes and cups that must survive drops: prefer R801N.
- Thin-walled, multi-cavity molds needing short cycles: prefer RJ870Z.
- Stiffness with stable clarity: R380Y.
Tips when switching grades
- Compare like with like: same test method and units (ISO/ASTM; MPa or kg/cm²; Izod or Charpy). Values from different methods are not directly comparable.
- Melt flow has a lot-to-lot tolerance – check the COA of the actual lot, not just the TDS.
- Different additives (nucleating, antistatic, antioxidant, slip) can change the part even when key values match.
- Always trial on your own machine and mold: check temperature, pressure, shrinkage, colour and appearance before switching volume.
FAQ
Can R380Y replace R801N?
They are close in MFR and tensile strength, so often yes, but R801N is tougher. If parts are prone to breaking on drops, trial before switching to R380Y.
Which random PP is clearest?
You cannot tell from TDS alone, because producers measure haze on different specimens and methods. Mold samples on your own tool to compare clarity.
How does random PP differ from homopolymer PP?
Random PP contains a small amount of comonomer (usually ethylene), making it clearer and more flexible but with lower heat resistance and stiffness than homopolymer.
Grade pages with TDS downloads: R380Y · R801N · RJ870Z
Other comparisons: PP homopolymer for injection, MFR 12 · PP impact copolymer for injection, MFR 9 · Are "5502" HDPE blow-molding grades from different producers the same? 5502 vs 5502BN vs Q5502BN vs HY55430 · General-purpose injection ABS
Based on producers' public TDS, for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).