SK impact PP copolymer for injection: B340F, B360F and B391G compared
Impact PP copolymers are used when injection-moulded parts must stay tough, even in the cold: battery cases, crates, boxes, appliance and automotive parts. This article compares three SK geo centric YUPLENE grades – B340F, B360F and B391G – from their TDS: the same HDT and Vicat, but clearly different flow and toughness.
Updated: 27 November 2026 · Thien An Plastics
Properties from the TDS
| Property | B340F SK geo centric (Korea) | B360F SK geo centric (Korea) | B391G SK geo centric (Korea) |
|---|---|---|---|
| PP type | Impact copolymer | Impact copolymer | Impact copolymer |
| Melt index (ASTM D1238) | 7.0 g/10 min | 16.0 g/10 min | 40.0 g/10 min |
| Tensile strength at yield | 270 kg/cm² (≈26.5 MPa) | 270 kg/cm² (≈26.5 MPa) | 260 kg/cm² (≈25.5 MPa) |
| Elongation at break | >500 % | >500 % | <500 % |
| Flexural modulus (ASTM D790) | 12,000 kg/cm² (≈1,177 MPa) | 12,000 kg/cm² (≈1,177 MPa) | 13,000 kg/cm² (≈1,275 MPa) |
| Notched Izod 23 °C | 15.0 kg·cm/cm (≈147 J/m) | 9 kg·cm/cm (≈88 J/m) | 7.5 kg·cm/cm (≈74 J/m) |
| Notched Izod -20 °C | 7.0 kg·cm/cm (≈69 J/m) | 3 kg·cm/cm (≈29 J/m) | 5.0 kg·cm/cm (≈49 J/m) |
| Dupont impact -10 °C | >30 kg·cm | >20 kg·cm | >20 kg·cm |
| Rockwell hardness (R) | 85 | 90 | 90 |
| HDT (ASTM D648) | 110 °C | 110 °C | 110 °C |
| Vicat softening point | 150 °C | 150 °C | 150 °C |
| Spiral flow (SK method) | 680 mm | >800 mm | >800 mm |
| Oven ageing 150 °C (ASTM D3012) | 360 hr | 360 hr | 360 hr |
| Features (TDS) | Excellent toughness; UL listed; battery cases | Excellent toughness; UL listed | High stiffness, very high flow; not chemically cracked – no surface gas marks |
Typical values from each producer's TDS, for reference only and not specifications. "—" means not published in the TDS. Values marked "≈" were converted by Thien An for easier comparison.
Key differences
- Flow: B340F has the lowest flow (MI 7), B360F is medium (16) and B391G very high (40) – B360F and B391G reach spiral flow above 800 mm versus 680 mm for B340F.
- Toughness: B340F is the toughest – Izod 15 kg·cm/cm at 23 °C and 7.0 at -20 °C, Dupont at -10 °C above 30 kg·cm; SK names battery cases as a use. B360F has the lowest -20 °C Izod (3).
- Stiffness: B391G is the stiffest (flexural modulus 13,000 kg/cm², Rockwell R90) despite its high flow; SK states it is not a chemically cracked grade, so it is free from surface gas marks.
- Common ground: all three have HDT 110 °C, Vicat 150 °C and 360 h oven ageing at 150 °C – the differences are mainly flow and impact.
Which grade to choose?
Notes when switching grades
- Moving from MI 7 to MI 40 requires lower melt temperature and injection pressure and a check for flash; the reverse needs more heat/pressure to fill.
- Cold impact differs widely (-20 °C Izod from 3 to 7) – run drop/impact tests at the real service temperature before switching for cold-use parts.
- The TDS use kg/cm² and kg·cm/cm; "≈" values are converted by Thien An. The HDT load is not stated, so compare only within the same producer.
- See also PP impact copolymer MFR 9.
FAQ
How do B340F, B360F and B391G mainly differ?
In flow and toughness: MI 7, 16 and 40; Izod at 23 °C of 15, 9 and 7.5 kg·cm/cm per the TDS. HDT and Vicat are the same.
Which grade is for battery cases?
B340F – SK’s TDS lists battery cases, and it has the highest impact in the group at both 23 °C and -20 °C.
Which grade suits thin-wall, hard-to-fill parts?
B391G – MI 40, spiral flow above 800 mm and the stiffest of the three; SK lists large and thin-wall products.
Where can I buy B340F, B360F, B391G with a TDS?
Thien An Plastics supplies B340F, B360F, B391G with TDS; contact +84 389 980 742 (WhatsApp, WeChat, Zalo) for a quote.
Grade pages (TDS download): B340F · B360F · B391G
More articles: PP impact copolymer MFR 4–5 · PP impact copolymer injection, MFR 9 · High-flow thin-wall PP compared
Based on producers' public TDS; for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).