PP for extrusion coating (woven bags, kraft paper, BOPP): 3375RM, F801C, L-270A, P838C and FC9415P compared
Coated PP woven bags (cement, rice, feed bags), PP-coated kraft paper and BOPP laminates all need a high-flow PP layer extruded directly onto the substrate – extrusion coating. The five grades below – 3375RM, F801C, L-270A, P838C and FC9415P – all have an MFR of 24–30 g/10 min but differ in PP type and stiffness.
Updated: 26 November 2026 · Thien An Plastics
Properties from the TDS
| Property | 3375RM IRPC (Thailand) | F801C Hyosung (Vietnam) | L-270A Lotte Chemical (Korea) | P838C SCG Chemicals (Thailand) | FC9415P TPC (Singapore) |
|---|---|---|---|---|---|
| PP type | Random copolymer | Homopolymer | Copolymer | Copolymer | Random copolymer |
| MFR (230 °C/2.16 kg) | 24 g/10 min | 25 g/10 min | 25 g/10 min | 26 g/10 min | 30 g/10 min |
| Density | — | 0.90 g/cm³ | 0.9 g/cm³ | 0.913 g/cm³ | 0.90 g/cm³ |
| Tensile strength at yield | 24 MPa | 340 kg/cm² (≈33.3 MPa) | 280 kgf/cm² (27 MPa) | 280 kg/cm² (≈27.5 MPa) | — |
| Flexural modulus | 750 MPa (1% secant) | 14,000 kg/cm² (≈1,373 MPa) | 9,800 kgf/cm² (970 MPa) | 11,000 kg/cm² (≈1,079 MPa) | 730 MPa (stiffness, ASTM D747) |
| Notched Izod impact (23 °C) | 3.5 J/m | 3.5 kg·cm/cm (≈34 J/m) | 4.5 kgf·cm/cm (44 J/m) | — | — |
| Rockwell hardness (R) | 86 | 95 | 96 | — | — |
| Melting point | — | — | 162 °C | 157 °C | 136 °C |
| Vicat softening point | — | — | 147 °C | 141 °C | — |
| Elongation | 35.5 % (yield) | — | >500 % (break) | 215 % (break) | 850 % (break) |
Typical values from each producer's TDS, for reference only and not specifications. "—" means not published in the TDS. Values marked "≈" were converted by Thien An for easier comparison.
Key differences
- Homopolymer or copolymer: F801C is a PP homopolymer and the stiffest (flexural modulus ≈1,373 MPa, Rockwell R95). 3375RM and FC9415P are random copolymers and softer (730–750 MPa); FC9415P has the lowest melting point (136 °C). L-270A and P838C are copolymers with medium stiffness (970–1,079 MPa).
- Flow: all 24–30 g/10 min; FC9415P is highest (30).
- Applications per TDS: 3375RM – coating BOPP film, woven bags, tarpaulins and paper, good adhesion, high clarity and high speed; F801C and L-270A – coating woven fabric and kraft paper, low neck-in, high-speed processing, good adhesion to paper, oil and moisture resistance (packaging for resin, fish, steel tube, dog food).
- Clarity: P838C lists a haze of 10 %; IRPC describes 3375RM as high clarity.
Which grade to choose?
Notes when switching grades
- Switching between homopolymer and copolymer changes coating stiffness, adhesion and brittleness – run peel tests and bag drop tests.
- Processing temperatures differ widely: F801C recommends a die at 290–300 °C, while 3375RM lists 190–240 °C – re-adjust temperatures when switching.
- Check neck-in and coating thickness at real line speed.
- For woven bags, see also PP raffia for woven bags.
FAQ
What is PP extrusion coating?
A high-flow PP (MFR about 24–30) extruded as a thin film and coated directly onto woven fabric, kraft paper or BOPP film for moisture and dust barrier and extra strength.
Which grade here is the stiffest?
F801C (Hyosung) – a PP homopolymer, flexural modulus 14,000 kg/cm² (≈1,373 MPa), Rockwell R95.
Which grade suits coating onto BOPP?
Per the TDS, 3375RM (IRPC) is used for coating BOPP film, woven bags, tarpaulins and paper, with high clarity and good adhesion.
Where can I buy coating PP with a TDS?
Thien An Plastics supplies 3375RM, F801C, L-270A, P838C and FC9415P with TDS; contact +84 389 980 742 (WhatsApp, WeChat, Zalo) for a quote.
Grade pages (TDS download): 3375RM · F801C · L-270A · P838C · FC9415P
More articles: PP raffia for woven bags: T3034, NSY114G, HP1102K, HY200, Y-130, HP550J and 1102K · PP for BOPP film: F3030 vs NSF113D vs UH622J vs UH625J vs 1104K · PP T3034 (Binh Son – BSR): properties and use in woven bags and FIBC
Based on producers' public TDS; for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).