PMMA (acrylic): ACRYREX CM-205 vs CM-207 compared
PMMA (polymethyl methacrylate, acrylic) is the clearest of the common plastics, with a hard, weather-resistant surface – used for lamp lenses, display covers, signs, glazing and clear housewares. This article compares Chi Mei’s ACRYREX CM-205 and CM-207 from their TDS.
Updated: 26 November 2026 · Thien An Plastics
Properties from the TDS
| Property | CM-205 Chi Mei (Taiwan) | CM-207 Chi Mei (Taiwan) |
|---|---|---|
| MVR (230 °C/3.8 kg, ISO 1133) | 1.8 cm³/10 min | 8.5 ml/10 min |
| Density | 1.19 | 1.19 g/cm³ |
| Tensile strength (ISO 527) | 68 MPa | 67 MPa |
| Elongation | 10.0 % | 8 % |
| Flexural strength (ISO 178) | 110 MPa | 97 MPa |
| Flexural modulus (ISO 178) | 3.2 GPa | 2.7 GPa |
| Charpy impact (23 °C) | 1.8 kJ/m² | 2 kJ/m² (notched) |
| Rockwell hardness | M95 | — |
| Vicat softening point | 115 °C (10 N) | 107 °C (1 kg); 99 °C (5 kg) |
| HDT (unannealed) | 84 °C | 89 °C (1.8 MPa); 100 °C annealed |
| UL 94 | HB (1.5 mm) | HB (1.5 mm) |
| Mould shrinkage | — | 0.2–0.6 % |
Typical values from each producer's TDS, for reference only and not specifications. "—" means not published in the TDS. Values marked "≈" were converted by Thien An for easier comparison.
Key differences
- Flow: CM-207 flows almost five times more than CM-205 (8.5 vs 1.8 cm³/10 min) – easier to injection mould, suited to thin walls and small detailed parts.
- Strength: CM-205 is the high-strength grade: flexural strength 110 MPa, modulus 3.2 GPa, elongation 10 % – higher than CM-207 (97 MPa, 2.7 GPa, 8 %).
- Heat: CM-205 has a Vicat of 115 °C (10 N) vs 107 °C (1 kg) for CM-207. HDT values are measured under different conditions in the two TDS.
- Both have density 1.19 and UL 94 HB at 1.5 mm.
Which grade to choose?
Notes when switching grades
- PMMA absorbs moisture – dry thoroughly before processing to avoid bubbles and silver streaks (see the producer’s drying guidance).
- Moving from CM-207 to CM-205 needs higher melt temperature/injection pressure because of much lower flow.
- PMMA is more brittle than PC (Charpy 1.8–2 kJ/m²); consider PC for parts with high impact loads.
- See also PC-1100U vs PC-110.
FAQ
Is PMMA the same as acrylic sheet?
Acrylic sheet is PMMA in sheet form; PMMA pellets such as CM-205 and CM-207 are used for sheet extrusion or injection moulding.
What is the main difference between CM-205 and CM-207?
Flow: 1.8 vs 8.5 cm³/10 min (230 °C/3.8 kg). CM-205 is stronger and more heat resistant; CM-207 is easier to injection mould.
PMMA or PC?
PMMA is clearer with a harder surface; PC is far tougher and more heat resistant. Choose by the part’s impact and temperature requirements.
Where can I buy CM-205, CM-207 with a TDS?
Thien An Plastics supplies CM-205, CM-207 with TDS; contact +84 389 980 742 (WhatsApp, WeChat, Zalo) for a quote.
Grade pages (TDS download): CM-205 · CM-207
More articles: Medium-viscosity polycarbonate: PC-1100U vs PC-110 compared · SAN resin (styrene acrylonitrile): INP576 (SAN 576), PN-127 and SAN 350HW compared · GPPS (crystal PS): GP150, GP525N, 500W, 525B and GPPS 535 compared
Based on producers' public TDS; for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).