EVA resin: EA28150, EVA 3522, LVS430 and 7350M compared (hot melt, foam, shoe soles)
The more vinyl acetate (VA) an EVA contains, the softer, more flexible and more adhesive it is. VA content and melt index (MI) are the two numbers that decide the grade. This article compares EA28150, EVA 3522, LVS430 and 7350M from their TDS – from very high-flow hot-melt EVA to shoe-sole foam EVA.
Updated: 26 November 2026 · Thien An Plastics
Properties from the TDS
| Property | EA28150 LG Chem (Korea) | EVA 3522 Sipchem (Saudi Arabia) | LVS430 Lotte Chemical (Korea) | 7350M Formosa Plastics (Taiwan) |
|---|---|---|---|---|
| Vinyl acetate content | 28 % | 22 wt% | 18 wt% | 18 % |
| Melt index (190 °C/2.16 kg) | 150 g/10 min | 3.5 g/10 min | 2.0 g/10 min | 2.5 g/10 min |
| Density | 0.946 g/cm³ | 0.944 g/cm³ | 0.940 g/cm³ | 0.938 g/cm³ |
| Tensile strength at break | 4.5 MPa | 9.6 MPa | 260 kgf/cm² (≈25.5 MPa) | 150 kg/cm² (≈14.7 MPa) |
| Elongation at break | 900 % | >800 % | 750 % | 800 % |
| Hardness Shore A / D | 74 / — | 78 / 32 | 92 / — | 88 / 38 |
| Melting point | 70 °C | 82 °C | 86 °C | 84 °C |
| Vicat softening point | — | 58 °C | 64 °C | 60 °C |
| Applications per TDS | Hot melt adhesive | Foam, extruded profiles, compounding | Foam, shoe soles, injection/sheet | Cross-linked foam shoes, midsoles, gaskets |
Typical values from each producer's TDS, for reference only and not specifications. "—" means not published in the TDS. Values marked "≈" were converted by Thien An for easier comparison.
Key differences
- EA28150 stands apart: VA 28 %, MI 150 – very high flow, melting 70 °C, for hot melt adhesives; LG Chem notes uniform VA and MI and good compatibility with other HMA raw materials.
- EVA 3522: VA 22 %, MI 3.5 – soft (Shore A 78) with good low-temperature toughness, for foam, extruded profiles and compounding.
- LVS430 and 7350M: both VA 18 %, MI 2.0–2.5 – the shoe-foam group. LVS430 has higher tensile strength at break (≈25.5 MPa) and is harder (Shore A 92); 7350M is for cross-linked foam shoes, midsoles and gaskets, brittleness point <−70 °C.
- Rule of thumb: higher VA means lower melting point, lower Vicat and lower hardness.
Which grade to choose?
Notes when switching grades
- Changing VA content changes hardness, foam expansion and cross-linking temperature – re-adjust the formulation (blowing agent, peroxide).
- EA28150’s MI (150) is dozens of times higher than the foam grades – they are not interchangeable.
- Producers measure VA and melting point by their own methods – compare relatively.
- Sipchem’s TDS states EVA 3522 is not intended for medical applications; ask the producer about food contact.
FAQ
What does a higher VA content do?
Higher VA makes EVA softer, more flexible, more adhesive and lower melting; e.g. EA28150 (VA 28 %) melts at 70 °C vs 86 °C for LVS430 (VA 18 %) per the TDS.
Which EVA is for hot melt?
LG Chem EA28150 – VA 28 %, MI 150, listed for hot melt adhesives.
Which EVA is for shoe soles?
LVS430 (Lotte; foam, shoe soles, sheet/injection) and 7350M (Formosa; cross-linked foam shoes, midsoles).
Where can I buy EA28150, EVA 3522, LVS430, 7350M with a TDS?
Thien An Plastics supplies EA28150, EVA 3522, LVS430, 7350M with TDS; contact +84 389 980 742 (WhatsApp, WeChat, Zalo) for a quote.
Grade pages (TDS download): EA28150 · EVA 3522 · LVS430 · 7350M
More articles: POE Exact 5171 (ExxonMobil): properties and use as a PP/PE impact modifier · Metallocene mLLDPE film grades: HP1018BN, D139FK, XP9200 and HPR3518CB compared · PP for CPP cast film: 1102M, HP2100L, H4540, UH513M and SFC-550 compared
Based on producers' public TDS; for technical reference only. For grade advice or a quote, contact Thien An Plastics: +84 389 980 742 (WhatsApp, WeChat, Zalo).